Synthesis, Stabilisation and Characterisation
CSIR NET: top-down and bottom-up routes, nucleation theory, LaMer model, citrate gold, hot injection, sol-gel, capping ligands, TEM, XRD-Scherrer and DLS.
- 22 min
On this page · 15 sections
- Prerequisites
- The Hook: Making a Billion Identical Crystals
- Top-Down versus Bottom-Up
- Classical Nucleation Theory
- The LaMer Model: Separate Nucleation from Growth
- Representative Syntheses
- Stabilisation: Keeping Particles Apart
- Characterisation: Which Technique Measures What
- Memory Tricks
- Don’t Confuse
- Common Mistakes
- Practice
- Quick Revision Table
- Key Takeaways
- What’s Next
Prerequisites
- Why small particles dissolve and large ones grow (Ostwald ripening): Nanoscale Size Effects and Surface Chemistry.
- Double layers, zeta potential and DLVO theory: Electrical Double Layer and Colloid Stability.
- Diffraction and line broadening: Bragg’s Law and X-ray Diffraction.
- Electron microscopy, XPS and EDX: Mass Spectrometry, Electron Spectroscopy and Microscopy.
- Soft-soft binding of thiols to gold: HSAB Concept.
The Hook: Making a Billion Identical Crystals
Top-Down versus Bottom-Up
| Top-down | Bottom-up | |
|---|---|---|
| Idea | carve or break a bulk solid into small pieces | build structures from atoms, ions or molecules |
| Examples | photolithography and electron-beam lithography; ball milling; laser ablation of a target; etching | chemical reduction of metal salts; sol–gel; hot-injection and heat-up colloidal synthesis; chemical vapour deposition; hydrothermal and solvothermal growth; microemulsion (reverse micelle) synthesis; self-assembly |
| Strengths | patterned, addressable structures; integrates with electronics | atomic-level control, narrow size distributions, cheap scale-up in solution |
| Weaknesses | resolution limits, surface damage, broad distributions from milling | ordered patterning over large areas is harder |
Classical Nucleation Theory
A new solid phase forms from a supersaturated solution (or vapour) only after a small cluster, a nucleus, has grown large enough to be stable. Forming a spherical cluster of radius \( r \) has two competing free-energy terms:
$$\Delta G(r) = 4\pi r^2\gamma - \frac{4}{3}\pi r^3\Delta G_v$$- \( 4\pi r^2\gamma \): the cost of creating an interface of energy \( \gamma \) per unit area (positive, wins at small \( r \));
- \( \frac{4}{3}\pi r^3\Delta G_v \): the gain from transferring material into the more stable phase, with \( \Delta G_v = RT\ln S/V_m \) per unit volume, where \( S \) is the supersaturation ratio and \( V_m \) the molar volume of the solid.
Setting \( \mathrm{d}\Delta G/\mathrm{d}r = 0 \):
$$\boxed{r^* = \frac{2\gamma}{\Delta G_v} = \frac{2\gamma V_m}{RT\ln S}, \qquad \Delta G^* = \frac{16\pi\gamma^3}{3\Delta G_v^2} = \frac{4}{3}\pi r^{*2}\gamma}$$Clusters smaller than the critical radius \( r^* \) tend to redissolve; larger ones tend to grow. The nucleation rate follows an Arrhenius-like form, \( J = A\exp(-\Delta G^*/k_BT) \). Because \( \Delta G^* \propto 1/(\ln S)^2 \), the rate is extraordinarily sensitive to supersaturation: below a critical supersaturation essentially no nuclei form, and above it they form in a burst.
Heterogeneous nucleation on a surface (a seed, a vessel wall, an impurity) has a lower barrier because part of the new interface replaces an existing one. Seeded growth exploits this: adding preformed seeds at a supersaturation too low for new nuclei makes the seeds grow without creating new particles.
The LaMer Model: Separate Nucleation from Growth
LaMer and Dinegar described the formation of monodisperse sulfur sols in 1950 with a plot of monomer concentration against time. It remains the standard explanation of how narrow size distributions arise.
graph LR
A["Stage I
monomer concentration rises
(precursor decomposes or is reduced)"] --> B["Stage II
concentration crosses critical
supersaturation: burst nucleation"]
B --> C["Concentration falls below
nucleation threshold:
no new nuclei form"]
C --> D["Stage III
existing nuclei grow by
diffusion of monomer"]The key is that nucleation happens in a short burst. All particles are born at nearly the same time and then grow together, so they finish at nearly the same size. If nucleation continues during growth, early and late nuclei end up at different sizes and the distribution broadens.
Growth: focusing and defocusing
- When growth is diffusion-limited and the solution is still well supersaturated, small particles grow faster in radius than large ones (\( \mathrm{d}r/\mathrm{d}t \propto 1/r \) for diffusion to a sphere), so the size distribution narrows (“focusing”).
- When the monomer is depleted, the supersaturation falls, the critical radius rises above the size of the smaller particles, and they begin to dissolve: Ostwald ripening sets in and the distribution broadens (“defocusing”).
Practical rule: to keep a distribution narrow, stop the reaction (cool it, or add more monomer) before ripening takes over.
Representative Syntheses
Metals by chemical reduction
| Method | Reagents and role | Typical product |
|---|---|---|
| Turkevich (citrate) method | HAuCl₄ in boiling water; trisodium citrate is both reducing agent and electrostatic stabiliser (adsorbed citrate makes the particles negatively charged) | Au spheres of roughly 10–20 nm, red sol; more citrate relative to gold gives smaller particles (Frens’ refinement) |
| Brust–Schiffrin two-phase method | AuCl₄⁻ moved from water into toluene by tetraoctylammonium bromide (phase-transfer agent), alkanethiol added (capping ligand), NaBH₄ (reducing agent) | thiolate-protected Au particles of a few nm (often 1–3 nm) that can be dried and redissolved like a molecular compound |
| Polyol method | metal salt heated in ethylene glycol or a similar polyol, which is solvent and reducing agent; PVP added as stabiliser and shape-directing agent | Ag, Pt, Pd particles, cubes and wires |
| Seed-mediated growth | small seeds (NaBH₄-reduced) added to a growth solution of metal salt, a mild reductant (ascorbic acid) and a surfactant (CTAB); a trace of AgNO₃ promotes rods for gold | gold nanorods with tunable aspect ratio |
| Borohydride reduction (strong reductant) | fast reduction gives many nuclei quickly | very small particles |
The strength of the reductant controls the balance of nucleation and growth. A strong reductant (NaBH₄) creates a high supersaturation and many small nuclei; a mild one (ascorbic acid in the presence of seeds) keeps supersaturation below the nucleation threshold so that only the seeds grow.
Semiconductor quantum dots: hot injection
In the hot-injection method developed for cadmium chalcogenide dots in the early 1990s (Bawendi’s group), a room-temperature solution of the chalcogen precursor (for example selenium dissolved in trioctylphosphine) is injected rapidly into a hot (roughly 250–350 °C) solution of a cadmium precursor in a coordinating solvent with long-chain ligands (trioctylphosphine oxide, oleic acid, alkylamines). Injection creates a sudden supersaturation and a nucleation burst; the temperature drop then stops further nucleation, and the dots grow slowly. Aliquots taken at increasing times have progressively red-shifted absorption and emission: a direct readout of growth through the Brus relation on the quantum confinement page. It is the LaMer picture carried out deliberately.
Core–shell dots are made by slowly adding shell precursors (for example zinc and sulfur sources) at a temperature too low to nucleate separate ZnS particles, so the shell grows epitaxially on the CdSe cores.
Oxides: sol–gel and the Stöber process
The sol–gel route builds an oxide network from metal alkoxides by hydrolysis and condensation:
$$\mathrm{Si(OEt)_4 + H_2O \longrightarrow Si(OEt)_3OH + EtOH} \quad \text{(hydrolysis)}$$$$\mathrm{\equiv Si{-}OH + HO{-}Si\equiv \longrightarrow \equiv Si{-}O{-}Si\equiv + H_2O} \quad \text{(water condensation)}$$$$\mathrm{\equiv Si{-}OEt + HO{-}Si\equiv \longrightarrow \equiv Si{-}O{-}Si\equiv + EtOH} \quad \text{(alcohol condensation)}$$- Acid catalysis favours hydrolysis over condensation and gives weakly branched, polymer-like chains that entangle into a gel.
- Base catalysis favours condensation at more highly condensed silicon and gives compact, highly branched clusters that grow into discrete particles.
The Stöber process (1968) is base-catalysed: TEOS in ethanol with water and ammonia gives monodisperse silica spheres, with size controlled by the water and ammonia concentrations. The wet gel can be dried by evaporation (a xerogel, which shrinks) or supercritically (an aerogel, which keeps its open pore network). Titanium, zirconium and aluminium alkoxides hydrolyse far faster than silicon alkoxides and usually need chelating modifiers (acetylacetone, acetic acid) to slow them.
Other bottom-up routes
- Microemulsions (reverse micelles): nanometre water droplets stabilised by a surfactant (AOT is a common example) in oil act as nanoreactors; the droplet size, set by the water-to-surfactant ratio \( w_0 \), limits particle size.
- Hydrothermal / solvothermal synthesis: heating precursors in water or another solvent in a sealed autoclave above its boiling point; common for oxide nanocrystals and zeolite-like frameworks.
- Chemical vapour deposition (CVD): gaseous precursors decompose on a heated substrate or catalyst; the main route to carbon nanotubes and large-area graphene (next page).
- Vapour–liquid–solid (VLS) growth: a liquid catalyst droplet (for example gold–silicon alloy) absorbs vapour-phase precursor, becomes supersaturated and precipitates a crystalline nanowire beneath itself; the droplet sets the wire diameter.
- Templates: pores of anodic aluminium oxide membranes or track-etched polymer films are filled electrochemically or chemically to give wires and tubes of the pore diameter.
- Biological and “green” routes: reduction of metal salts with plant extracts, sugars or microorganisms; attractive for low toxicity and cost, but size control is usually poorer.
Stabilisation: Keeping Particles Apart
Nanoparticles have a large surface energy and strong van der Waals attraction, so without protection they aggregate irreversibly. Two mechanisms, often combined, keep them dispersed:
| Mechanism | How it works | Examples | Weakness |
|---|---|---|---|
| Electrostatic | adsorbed ions give a surface charge; overlapping double layers repel (DLVO) | citrate on gold; charged oxide surfaces at pH away from the isoelectric point | fails at high ionic strength (double layer compressed) or near the isoelectric point |
| Steric | adsorbed or bound chains resist interpenetration (osmotic and entropic repulsion) in a good solvent | PVP, PEG, thiols, oleic acid/oleylamine, phosphines | fails in a poor solvent for the chains |
| Electrosteric | charged polymers or charged ligands combine both | polyelectrolytes, proteins | — |
A zeta potential of magnitude above about 30 mV is a widely used rule of thumb for a well-stabilised electrostatic dispersion; it is a guideline, not a law. Adding salt to a citrate-gold sol screens the charge and turns it from red to blue as the particles aggregate (see the plasmon coupling on the optical properties page). The full theory is on Electrical Double Layer and Colloid Stability.
Ligands and self-assembled monolayers
Capping ligands do more than prevent aggregation: they passivate surface states (quantum dots), control which crystal faces grow (shape control) and set solubility (oleic-acid-capped dots dissolve in hexane; after exchange with a charged thiol they dissolve in water).
Alkanethiols on gold are the classic self-assembled monolayer (SAM). The thiol binds strongly to gold as a thiolate (a soft–soft interaction), and van der Waals attraction between long alkyl chains drives them into a dense, ordered, tilted monolayer. On flat Au(111) surfaces, long-chain thiol SAMs are commonly described with chains tilted at about 30° from the surface normal. The terminal group (–CH₃, –OH, –COOH, –NH₂) sets the wettability and chemistry of the new surface, which is why SAMs are used to build sensors and to anchor biomolecules.
graph TD
A["Precursor + reductant
or alkoxide + water"] --> B["Nucleation burst
(LaMer stage II)"]
B --> C["Growth
(focusing while supersaturated)"]
C --> D["Capping ligand binds:
growth slowed, shape set,
aggregation prevented"]
D --> E["Purification and
ligand exchange"]
E --> F["Characterisation
TEM, XRD, DLS, UV-Vis"]Characterisation: Which Technique Measures What
| Technique | What it gives | Size it reports | Notes |
|---|---|---|---|
| TEM / HRTEM | size and shape of individual particles; lattice fringes; electron diffraction (SAED) for crystal structure | inorganic core (ligands nearly invisible) | counts hundreds of particles to build a histogram; samples dried on a grid |
| SEM | morphology of larger structures and films; with EDX, elemental composition | outer surface | lower resolution than TEM for small particles |
| AFM | topography; particle height on a flat substrate | height is reliable; lateral size broadened by the tip | works in air or liquid |
| STM | atomic-resolution images of conducting surfaces | — | tunnelling current falls exponentially with gap |
| XRD (Scherrer) | phase identification; crystallite size from peak broadening | coherently diffracting domain | a lower bound to particle size; small at 1–2 nm, insensitive above ~100 nm |
| DLS | hydrodynamic diameter from diffusion coefficient; a dispersity index | core + ligand shell + solvation layer | intensity-weighted, dominated by large particles and aggregates |
| Zeta potential | electrophoretic mobility, surface charge | — | predicts electrostatic stability |
| UV–visible | plasmon band (metals) or excitonic peak (dots); sizes via calibration | — | quick check of size, shape and aggregation |
| Photoluminescence | emission wavelength, width, quantum yield | — | quantum dots, carbon dots |
| BET gas adsorption | specific surface area and porosity | equivalent sphere size \( 6/\rho S \) | powders |
| XPS | surface composition and oxidation states (top few nm) | — | detects oxidised surfaces, bound ligands |
| TGA | mass of organic ligand per particle | — | ligand density |
| Raman | vibrational fingerprints; carbon nanotube and graphene analysis | — | see next page |
The Scherrer equation
Small crystallites broaden diffraction peaks because fewer lattice planes contribute to destructive interference away from the exact Bragg angle. The mean crystallite dimension \( \tau \) normal to the diffracting planes is
$$\boxed{\tau = \frac{K\lambda}{\beta\cos\theta}}$$- \( K \) = shape factor, about 0.9 for roughly spherical crystallites;
- \( \lambda \) = X-ray wavelength (Cu Kα: 0.15406 nm);
- \( \beta \) = peak width (full width at half maximum) in radians, after subtracting instrumental broadening;
- \( \theta \) = Bragg angle, half of the measured \( 2\theta \).
Strain and defects also broaden peaks, so Scherrer sizes are best read as lower bounds. A particle made of several crystalline domains (twinned gold particles are common) gives a Scherrer size smaller than its TEM diameter.
Dynamic light scattering and the Stokes–Einstein equation
DLS measures the fluctuations in scattered intensity caused by Brownian motion, extracts the translational diffusion coefficient \( D \), and converts it into a hydrodynamic radius:
$$\boxed{D = \frac{k_BT}{6\pi\eta r_H}}$$Counting atoms and particles
Gold has 59.0 atoms per nm³ (from \( \rho = 19.3 \) g cm⁻³ and 196.97 g mol⁻¹). A sphere of diameter \( d \) therefore contains \( 59.0 \times \pi d^3/6 \) atoms:
| \( d \) / nm | 2 | 5 | 15 |
|---|---|---|---|
| Au atoms per particle | about 250 | about 3,900 | about 104,000 |
If 0.25 mM HAuCl₄ is reduced completely to 15 nm particles, the particle concentration is \( 0.25 \times 10^{-3}/104{,}000 = 2.4 \times 10^{-9} \) M, i.e. 2.4 nM. Nanoparticle concentrations are nanomolar even when the gold concentration is sub-millimolar.
STM: why it resolves atoms
The tunnelling current between tip and sample decays as \( I \propto e^{-2\kappa d} \), with \( \kappa = \sqrt{2m_e\phi}/\hbar \) for a barrier of height \( \phi \) (roughly the work function). For \( \phi = 4.5 \) eV, \( \kappa = 10.9 \) nm⁻¹; a change of 0.1 nm in the gap changes the current by \( e^{2.17} \approx 8.8 \), nearly an order of magnitude. Because almost all the current flows through the outermost atom of the tip, lateral atomic resolution is possible. The underlying tunnelling problem is the barrier penetration treated on Particle in a Box, Harmonic Oscillator and Tunnelling.
Memory Tricks
Don’t Confuse
| This | vs | That |
|---|---|---|
| Nucleation (new particles form; needs \( S \) above a critical value) | Growth (existing particles enlarge; occurs at lower \( S \)) | |
| Homogeneous nucleation (in the bulk solution) | Heterogeneous nucleation (on seeds or surfaces; lower barrier) | |
| Ostwald ripening (dissolution–redeposition) | Aggregation (particles stick on contact) | |
| Electrostatic stabilisation (sensitive to salt) | Steric stabilisation (sensitive to solvent quality) | |
| Crystallite size (XRD) | Particle size (TEM) and hydrodynamic size (DLS) | |
| Xerogel (dried by evaporation, shrinks) | Aerogel (supercritically dried, highly porous) | |
| CVD (gas precursors react on a surface) | VLS (vapour dissolves in a liquid droplet that precipitates a wire) |
Common Mistakes
Practice
All questions below are original practice questions written for this page. They are not from any CSIR NET paper.
Level 1: Foundation
- Classify as top-down or bottom-up: ball milling, Stöber synthesis, electron-beam lithography, CVD growth of nanotubes.
- Write the expressions for the critical radius and the barrier height in classical nucleation theory.
- What does tetraoctylammonium bromide do in the Brust–Schiffrin synthesis?
Answers
- Ball milling and electron-beam lithography: top-down. Stöber synthesis and CVD growth: bottom-up.
- \( r^* = 2\gamma/\Delta G_v = 2\gamma V_m/(RT\ln S) \); \( \Delta G^* = 16\pi\gamma^3/3\Delta G_v^2 \).
- It is the phase-transfer agent that carries AuCl₄⁻ from water into toluene, where reduction in the presence of thiol takes place.
Level 2: Part B Style
Practice Q1. In classical nucleation theory, if the supersaturation ratio is raised so that \( \ln S \) triples (all else constant), the nucleation barrier \( \Delta G^* \):
(a) triples (b) falls to one-third (c) falls to one-ninth (d) falls to one-twenty-seventh
Answer: (c)
\( \Delta G^* \propto 1/\Delta G_v^2 \propto 1/(\ln S)^2 \): tripling \( \ln S \) divides the barrier by 9. The critical radius falls to one-third (option (b) describes \( r^* \), not the barrier).
Practice Q2. A Cu Kα (λ = 0.15406 nm) diffraction peak of a ZnO nanopowder appears at \( 2\theta = 36.3° \) with a corrected FWHM of 0.80°. The crystallite size (K = 0.9) is closest to:
(a) 5.2 nm (b) 10.4 nm (c) 12.3 nm (d) 0.18 nm
Answer: (b) 10.4 nm
\( \theta = 18.15° \), \( \cos\theta = 0.9502 \), \( \beta = 0.80 \times \pi/180 = 0.01396 \) rad. \( \tau = 0.9 \times 0.15406/(0.01396 \times 0.9502) = 10.4 \) nm.
Option (c) uses \( \cos 2\theta \) instead of \( \cos\theta \); option (d) leaves \( \beta \) in degrees; option (a) doubles the width (for example, mistaking the FWHM for the half width).
Practice Q3. In the Turkevich synthesis of gold nanoparticles, trisodium citrate acts as:
(a) reducing agent only (b) stabiliser only (c) both reducing agent and stabiliser (d) phase-transfer agent
Answer: (c)
Citrate reduces Au(III) in boiling water and the adsorbed citrate anions charge and stabilise the particles.
Practice Q4. Base-catalysed hydrolysis and condensation of TEOS in ethanol–water–ammonia (the Stöber process) mainly gives:
(a) linear, weakly branched siloxane chains that form a transparent gel (b) monodisperse spherical silica particles (c) crystalline quartz nanowires (d) mesoporous silica only in the absence of water
Answer: (b)
Base catalysis favours condensation into compact, highly branched clusters that grow into discrete spheres. Option (a) describes acid catalysis.
Level 3: Part C Style
Practice Q5. Citrate-capped gold particles are characterised by three methods. TEM gives a mean core diameter of 15 nm. DLS in water at 298.15 K (\( \eta = 0.890 \) mPa s) gives \( D = 2.6 \times 10^{-11} \) m² s⁻¹. The Au(111) peak gives a Scherrer size of 9 nm. Which conclusions are justified?
- The hydrodynamic diameter is about 19 nm.
- The DLS size exceeds the TEM size because DLS includes the ligand and solvation shell and is intensity-weighted.
- The Scherrer size smaller than the TEM size suggests that particles contain more than one crystalline domain (or strain).
- Each 15 nm particle contains about \( 1.0 \times 10^5 \) gold atoms.
(a) 1 and 2 only (b) 2 and 3 only (c) 1, 2 and 3 only (d) 1, 2, 3 and 4
Answer: (d) 1, 2, 3 and 4
- \( r_H = k_BT/(6\pi\eta D) = 4.117 \times 10^{-21}/(6\pi \times 0.890 \times 10^{-3} \times 2.6 \times 10^{-11}) = 9.4 \times 10^{-9} \) m; \( d_H = 18.9 \) nm ≈ 19 nm. Correct.
- Correct: the usual reason DLS > TEM.
- Scherrer gives the coherently diffracting domain size; twinned (multiply twinned) gold particles and strain broaden peaks, giving a smaller size. Correct.
- \( 59.0 \times \pi(15)^3/6 = 1.04 \times 10^5 \). Correct.
Practice Q6. A nucleation study uses \( \gamma = 0.10 \) J m⁻², \( V_m = 3.0 \times 10^{-5} \) m³ mol⁻¹ and 298.15 K. Which statements are correct?
- At \( S = 10 \) the critical radius is about 1.05 nm.
- At \( S = 10 \) the barrier is about 112 \( k_BT \), so homogeneous nucleation is negligible.
- Raising \( S \) to 100 lowers the barrier to about 28 \( k_BT \) and the critical nucleus to about 12 formula units.
- Adding seeds at \( S = 10 \) leads to growth of the seeds rather than new nucleation.
(a) 1 and 3 only (b) 1, 2 and 3 only (c) 2 and 4 only (d) 1, 2, 3 and 4
Answer: (d) 1, 2, 3 and 4
- \( \Delta G_v = RT\ln S/V_m = 2479 \times 2.3026/3.0 \times 10^{-5} = 1.90 \times 10^8 \) J m⁻³; \( r^* = 0.20/1.90 \times 10^8 = 1.05 \) nm. Correct.
- \( \Delta G^* = \tfrac{4}{3}\pi r^{*2}\gamma = 4.63 \times 10^{-19} \) J; divided by \( k_BT = 4.12 \times 10^{-21} \) J gives 112. \( e^{-112} \) is vanishingly small. Correct.
- \( \ln S \) doubles: \( \Delta G^* \) quarters to 28 \( k_BT \); \( r^* = 0.53 \) nm, volume \( 6.1 \times 10^{-28} \) m³, \( \times N_A/V_m = 12 \) units. Correct.
- Seeds already exceed the critical size and need no barrier crossing; growth consumes monomer without new nuclei. Correct. This is the logic of seed-mediated growth.
Practice Q7. Aliquots are removed during a hot-injection CdSe synthesis at 1, 5 and 20 minutes. Their first excitonic absorption peaks are at 500, 545 and 580 nm, and the emission linewidth is narrowest at 5 minutes and broader at 20 minutes. The most consistent interpretation is:
(a) The dots shrink with time; ripening narrows the distribution at long times. (b) The dots grow with time; growth focuses the distribution early, and ripening defocuses it later as monomer is depleted. (c) New nuclei form continuously; the peak shifts because of solvent evaporation. (d) The dots grow with time; the broadening at 20 minutes is caused by the Coulomb term in the Brus equation.
Answer: (b)
A red-shifting excitonic peak means a shrinking gap, i.e. larger dots (confinement \( \propto 1/R^2 \)). Early diffusion-limited growth at high supersaturation narrows the distribution; once monomer is used up, Ostwald ripening broadens it. The Brus Coulomb term affects peak position, not width.
Quick Revision Table
| Topic | Key point |
|---|---|
| Top-down | lithography, milling, etching, laser ablation (mostly) |
| Bottom-up | reduction, sol–gel, hot injection, CVD, VLS, microemulsion, hydrothermal, self-assembly |
| Nucleation | \( r^* = 2\gamma V_m/RT\ln S \); \( \Delta G^* = 16\pi\gamma^3/3\Delta G_v^2 = \tfrac{1}{3}(4\pi r^{*2}\gamma) \) |
| LaMer | burst nucleation, then growth without new nuclei |
| Growth | focusing (diffusion-limited, high \( S \)) vs defocusing (ripening, low \( S \)) |
| Turkevich | HAuCl₄ + citrate (reductant + stabiliser), boiling water |
| Brust–Schiffrin | TOAB (phase transfer), thiol (cap), NaBH₄ (reductant), toluene |
| Nanorods | seeds + CTAB + ascorbic acid + AgNO₃ |
| Hot injection | rapid injection → burst; temperature drop → growth only |
| Sol–gel | acid: chains, gels; base: particles (Stöber) |
| Stabilisation | electrostatic (salt-sensitive), steric (solvent-sensitive) |
| Scherrer | \( \tau = K\lambda/\beta\cos\theta \), \( \beta \) in radians, \( \theta = 2\theta/2 \) |
| DLS | \( r_H = k_BT/6\pi\eta D \); \( d_H > d_{\text{TEM}} \) |
| Au atoms | 59.0 nm⁻³; 15 nm sphere ≈ \( 1.04 \times 10^5 \) atoms |
| STM | \( I \propto e^{-2\kappa d} \); 0.1 nm → factor ≈ 9 |
Key Takeaways
What’s Next
- Carbon and Two-Dimensional Nanomaterials: fullerenes, nanotubes, graphene and the applications of nanomaterials.
- Surface area from gas adsorption, used to check particle size: Adsorption Isotherms and Surface Area.
- Thermal methods that quantify ligand loading: Thermoanalytical Methods.
- Nanoscience and Technology: Quick Revision.